검색결과

검색조건
좁혀보기
검색필터
결과 내 재검색

간행물

    분야

      발행연도

      -

        검색결과 2

        2.
        2013.04 KCI 등재 구독 인증기관 무료, 개인회원 유료
        In this study, carbon/epoxy composite DCB(double cantilever beam) specimens based on K-means clustering and wavelet transform analyses are presented. For the fracture Mode I, the fiber orientation θ = [0 ]24 and θ = [±45]12 both shown up stable crack growth in DCB testing. For the fiber orientation θ = [0 ]24 , the continuous type AE signal showed at central frequency 130~270kHz, which means that matrix micro cracking was occurred. The Burst type AE signal was occurred at central frequency 200~300kHz due to fiber bridging and fiber breaking. Other burst type AE signals were occurred at central frequency 130~180kHz with very high amplitude due to fiber bridging. For the fiber orientation θ = [±45]12 , the burst type signal showed at central frequency 220~300kHz, which means that fiber breaking was occurred. Mixed type of burst and continuous signals were captured at central frequency 250~480kHz due to fiber friction.
        4,000원