검색결과

검색조건
좁혀보기
검색필터
결과 내 재검색

간행물

    분야

      발행연도

      -

        검색결과 2

        1.
        2006.09 구독 인증기관·개인회원 무료
        WC-10Co-0.8VC nanocrystalline powders were sintered by spark plasma sintering (SPS) and hot press sintering (HPS), and the microstructure and properties were compared. Results show that dense WC-10Co-0.8VC can be obtained by SPS in several minutes when the sintering temperature is >1200℃. Sintered at a temperature of 1300℃, the sample prepared by SPS for 3 minutes has higher density, finer grains and better properties than that prepared by HPS for 60 minutes. SPS can be used to prepare nanocrystalline WC-10Co-0.8VC with improved properties when suitable sintering parametesr are chosen.